Pinus monticola

 

 

click here for the page in Engilsh units of measure

this page uses metric units of measure

 

Family: Pinaceae

 

 

 

 

 

 

click to print or download the file in .pdf format

 

Western White Pine

 

 

 

 

The genus Pinus is composed of about 100 species native to temperate and tropical regions of the world. Wood of pine can be separated microscopically into the white, red and yellow pine groups. The word pinus is the classical Latin name. The word monticola means inhabiting mountains.

Other Common Names: Berg-tall, Columbia pijn, finger-cone pine, Idaho white pine, little sugar pine, mountain pine, mountain white pine, Norway white pine, pin argente, pin argente americain, pino bianco americano, pino blanco americano, silver pine, soft pine, vasterns Weymouth-tall, western white pine, Weymouth berg-pijn, Weymouth mountain pine, white pine, yellow pine.

Distribution: Western white pine is native to the mountains ffrom northwestern Montana, extreme southwestern Alberta and southern British Columbia, south to Washington, Oregon and California through the Sierra Nevada to western Nevada and central California.

The Tree: Western white pine trees reach heights of 180 feet, with a clear bole for 70 to 100 feet and diameters of 3.5 feet. Over mature trees may reach heights of 197 feet, with diameters of almost 6 feet. They may grow for 300 to 400 years.

General Wood Characteristics: The sapwood of western white pine is nearly white to pale yellow, while the heartwood is cream to light reddish brown and may turn darker upon exposure. The wood has a slight resinous odor, but no characteristic taste. It is straight grained and has a rather coarse texture. It is also soft, light, is moderately weak in bending, moderately strong in end compression and moderately low in shock resistance. It works well with tools, glues well and holds paint very well. It does not split when nailed, but has medium nail holding ability. It is easy to dry, has moderate shrinkage and stays in place well after proper drying. It is low in decay resistance.

 

 

 

Mechanical Properties (2-inch standard)

 

 

 

 

Compression

 

 

 

 

Specific

gravity

MOE

GPa

MOR

MPa

Parallel

MPa

Perpendicular

MPa

WMLa

Kj/m3

Hardness

N

Shear

MPa

Green

0.35

8.20

32.4

16.7

1.31

34.5

1160

4.69

Dry

0.42

10.1

66.9

34.7

3.24

60.7

1870

7.17

aWML = Work to maximum load.

Reference (56).

 

Drying and Shrinkage

Type of shrinkage

Percentage of shrinkage
(green to final moisture content)

0% MC

6% MC

20% MC

Tangential

7.4

5.9

2.5

Radial

4.1

3.3

1.4

Volumetric

11.8

9.4

3.9

References: (178, 56, 192).

Kiln Drying Schedulesa

 

Conventional temperature/moisture content-controlled schedulesa


Condition

4/4, 5/4
stock

6/4 stock

8/4
stock

10/4
stock

12/4
stock

British schedule
4/4 stock

Lower grades

T9-C6

NA

T7-C6

NA

NA

NA

Upper grades

T9-C5

T7-C5

T7-C4

T5-C4

T8-C3

L

aReference (28, 185).

 

Conventional temperature/time-controlled schedulesa

 

Lower grades

Upper grades


Condition

4/4, 5/4 stock

6/4 stock

8/4 stock

4/4, 5/4 stock

6/4 stock

8/4 stock

12/4, 16/4 stock

Standard

295

301

301

295

301

301

NA

aReferences (28, 185).

 

Working Properties: It works well with tools, glues well and holds paint very well. It does not split when nailed, but has medium nail holding ability.

Durability: It is rated as slightly or nonresistant to heartwood decay.

Preservation: No information available at this time.

Uses: Matches, boxes, crates, wall and roof sheathing, interior paneling, windows, panel doors, trim, moldings, cut stock, foundry patterns, furniture, laminated roof decking, plywood, veneer, pulp, paper and particle board.

Toxicity: In general, working with pine wood may cause dermatitis, allergic bronchial asthma or rhinitis in some individuals (5,9&13).

 

Additional Reading and References Cited (in parentheses)

1. Boone, R. S.; Kozlik, C. J.; Bois, P. J., and Wengert, E. M. Dry kiln schedules for commercial woods - temperate and tropical. Madison, WI: USDA Forest Service, FPL-GTR-57; 1988.

2. Dallimore, W.; Jackson, A. B., and Harrison, S. G. A handbook of Coniferae and Ginkgoaceae. London, UK: Edward Arnold Ltd.; 1966.

3. Elias, T. S. The complete trees of North America, field guide and natural history. New York, NY: van Nostrand Reinhold Co.; 1980.

4. Graham, R. T. Pinus monticola Dougl. ex D. Don. Western White Pine. in: Burns, R. M. and Honkala, B. H., tech. coords. Silvics of North America. Volume 1, Conifers. Washington, DC: USDA Forest Service; 1990; pp. 385-394.

5. Hausen, B. M. Woods injurious to human health. A manual. New York, NY: Walter de Gruyter; 1981.

6. Henderson, F. Y. A handbook of softwoods. London: HMSO; 1977.

7. Little, jr. E. L. Checklist of United States trees (native and naturalized). Washington, DC: USGPO, USDA Forest Service, Ag. Handbook No. 541; 1979.

8. Lowery, D. P. Western White Pine, an American wood. Washington, DC, USA.: USDA Forest Service, FS-258.; 1984.

9. Mitchell, J. and Rook, A. Botanical dermatology: plants and plant products injurious to the skin. Vancouver, BC: Greenglass Ltd.; 1979.

10. Simpson, W. T. Dry kiln operator's manual. Madison, WI: USDA Forest Service, FPL Ag. Handbook No. 188; 1991.

11. Summitt, R. and Sliker, A. CRC handbook of materials science. Vol. 4. Boca Raton, FL: CRC Press, Inc.; 1980.

12. USDA. Wood handbook: wood as an engineering material. Madison, WI: USDA Forest Service, FPL Ag. Handbook No. 72; 1974.

13. Woods, B. and Calnan, C. D. Toxic woods. British Journal of Dermatology. 1976; 95(13):1-97.